C93600 Material Data Sheet

Chemical Properties -- C93600 Bronze, Mod SAE 64, Leaded Tin Bronze

Element

Nominal %

Minimum %

Maximum %

Aluminum

-

-

0.005

Antimony

-

-

0.55

Copper

81

81

85

Iron

-

-

0.2

Lead

12

11

13

Nickel

-

-

1

Phosphorus

-

-

0.15

Silicon

-

-

0.005

Sulfur

-

-

0.08

Tin

7

6

8

Zinc

-

-

1

 

Mechanical Properties -- C93600 Bronze, Mod SAE 64, Leaded Tin Bronze

M02 - As Centrifugal Cast

 

Tensile Strength:

Minimum 35 ksi

Yield Strength:

Minimum 21 ksi - 0.5% Ext. under load

Elongation:

15%, in 2 inches

 

 

M07 - As Continuous Cast

 

Tensile Strength:

Minimum 33 ksi

Yield Strength:

Minimum 20 ksi - 0.5% Ext. under load

Elongation:

10%, in 2 inches

 

Physical Properties -- C93600 Bronze, Mod SAE 64, Leaded Tin Bronze

Property

US Customary

Melting Point - Liquidus

1720 F

Melting Point - Solidus

1550 F

Density

0.325 lb/in3 at 68 F

Specific Gravity

9

Specific Heat Capacity

0.09 Btu/lb/oF at 68 F

Coefficient of Thermal Expansion

10.3 ·10-6 per oF (68-392 F)

Thermal Conductivity

28.5 Btu · ft/(hr · ft2·oF)at 68F

Electrical Conductivity

11 %IACS @ 68 F

Modulas of Elasticity in Tension

14,000 ksi

 

Fabrication Properties -- C93600 Bronze, Mod SAE 64, Leaded Tin Bronze

Joining Methods

Suitability

Soldering

Good

Brazing

Good

Oxyacetylene Welding

Not Recommended

Gas Shielded Arc Welding

Not Recommended

Coated Metal Arc Welding

Not Recommended

Machinability (C360 Brass =100)

80